Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® A3EG3 - PA66-GF15 - BASF

Material Data Center offers the following functions for Ultramid® A3EG3:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Caractéristiques des transformations/physiquessec / condUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 70 / * cm³/10min ISO 1133
Température 275 / * °C -
Charge 5 / * kg -
ASTM Data
Retrait au moulage , parallèle 0.0055 mm/mm ASTM D 955
Propriétés mécaniquessec / condUnitéNorme du test
ISO Data
Module en traction 6000 / 4500 MPa ISO 527
Contrainte d'écoulement 130 / 85 MPa ISO 527
Déformation nominale à la rupture 3 / 10 % ISO 527
Module de flexion, 23°C 5500 / 4000 MPa ISO 178
Module de fluage en traction, 1000h * / 2500 MPa ISO 899-1
Résistance au choc Charpy, +23°C 45 / 70 kJ/m² ISO 179/1eU
Résistance au choc Charpy, -30°C 43 / - kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C 8 / 11 kJ/m² ISO 179/1eA
Résistance au choc Charpy (entaillé), -30°C 7 / - kJ/m² ISO 179/1eA
Résistance au choc Izod avec entaille, +23°C 5.5 / 6.5 kJ/m² ISO 180/1A
Ball indentation hardness 200 / 150 MPa ISO 2039-1
ASTM Data
Résistance de traction à la rupture 114 / - MPa ASTM D 638
Allongement à la rupture 3 / - % ASTM D 638
Module de flexion 5170 / - MPa ASTM D 790
Izod choc avec entaille, 1/8 in 59 / - J/m ASTM D 256
Izod choc avec entaille, bas température 53 / - J/m ASTM D 256
Température -40 °C -
Propriétés thermiquessec / condUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 260 / * °C ISO 11357-1/-3
Température de fléchissement s/chrg, 1.80 MPa 250 / * °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 250 / * °C ISO 75-1/-2
Coeffic. de dilatation therm. linéique, parallèle 32 / * E-6/K ISO 11359-1/-2
Coeffic. de dilatation therm. linéique, perpend. 75 / * E-6/K ISO 11359-1/-2
Inflammabilité ep. nom. 1.5 mm HB / * class IEC 60695-11-10
Epaisseur de l'éprouvette 1.6 / * mm -
ASTM Data
DTUL à 66 psi 250 °C ASTM D 648
DTUL à 264 psi 250 °C ASTM D 648
Température de fusion 260 °C ASTM D 3418
Propriétés électriquessec / condUnitéNorme du test
ISO Data
Permittivité relative, 1MHz 3.5 / 5.5 - IEC 62631-2-1
Facteur de pertes, 1MHz 140 / 1600 E-4 IEC 62631-2-1
Résistivité transversale 1E13 / 1E10 Ohm*m IEC 62631-3-1
Résistivité superficielle * / 1E10 Ohm IEC 62631-3-2
Indice de résistance au cheminement 550 / - - IEC 60112
ASTM Data
Résistance volumique 1E13 / - Ohm*cm ASTM D 257
Propriétés diversessec / condUnitéNorme du test
Absorption d'eau 7 / * % Sim. to ISO 62
Absorption d'humidité 2.2 / * % Sim. to ISO 62
Masse volumique 1230 / - kg/m³ ISO 1183
Absorption d’eau, équilibre 7 % ASTM D 570
Densité 1240 kg/m³ ASTM D 792
Propriétés spécifiques à la matièresec / condUnitéNorme du test
ISO Data
Indice de viscosité 145 / * cm³/g ISO 307, 1157, 1628
Caractéristiques
Transformation
Moulage par injection, Extrusion (autres)
Conditionnement
Granulés, Couleurs naturelles
Applications
Automobile, Électrotechnique et électrique
Disponibilité régionale
Amérique du nord, Asia Pacific
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.